Short answer: a fused silica tube does not have one pressure rating. The safe pressure depends on inner diameter, wall thickness, temperature, surface condition, how the ends are closed, and whether the load is steady or cycling. This guide shows the two calculations that matter, internal pressure (hoop stress) and external pressure or vacuum (buckling), with worked numbers, so you can judge whether a tube is in the right range before you send a drawing for a quote.

The tables below are theoretical screening values, not working pressures or a certified rating. Any pressurized glass part needs a safety factor, a containment plan and a review by someone accountable for the system.

Why there is no single pressure rating for a quartz tube

Search results for “high pressure quartz tube” often quote one pressure per wall thickness, as if a 3 mm wall always holds the same pressure. It does not. For the same wall, a larger diameter carries a higher stress, because the pressure pushes on a larger area. The rating therefore has to be calculated for the exact tube.

FGQuartz handles it the same way: on our custom quartz glass tubes the pressure or vacuum wall thickness is calculated per drawing from OD, wall, temperature and end closures, and it is not a catalog number.

The material numbers behind the calculation

Fused silica is a brittle glass. It is very strong in compression and much weaker in tension, and its tensile strength is controlled by surface flaws rather than by the bulk. That is why designers use a derated design stress, not the theoretical strength.

Property (20 °C unless noted) Value used here
Design tensile strength 48 MPa (about 7,000 psi)
Compressive strength 1,100 MPa
Flexural strength 67 MPa
Young’s modulus 72 GPa
Poisson’s ratio 0.17
Thermal expansion (20–300 °C) about 5.5 × 10−7 /°C
Continuous service / softening about 1,200 °C / about 1,680 °C

These values match the data on our fused silica specifications page. For background on the material itself, see what quartz glass is.

Two behaviors matter for pressure work:

  • Flaws set the limit. A scratch, chip or micro-crack on the surface that sees tension is where a tube fails. Surface finish, handling and cleaning matter as much as wall thickness.
  • Load duration matters. Glass held under sustained tension can fail at a lower stress than in a short test, especially in humid air. A tube that holds pressure for a minute is not proven for a year of steady load.

Internal pressure: hoop stress in a quartz tube

When a tube is pressurized from inside, the highest tensile stress is the hoop stress at the inner wall. For thin walls the common approximation is:

S = p × r / t

where S is hoop stress, p is internal pressure, r is inside radius and t is wall thickness (consistent units). A published rupture formula for fused quartz tubing from another manufacturer uses the same form (Finkenbeiner, see references). For heavier walls, the exact Lamé result for the inner-wall stress is better:

S = p × (ro2 + ri2) / (ro2 − ri2)

where ro and ri are outside and inside radius. Solving for pressure at the 48 MPa design stress gives the upper bounds below.

ID (mm) Wall (mm) Upper bound at 48 MPa In bar
20 2 8.7 MPa 87
50 3 5.4 MPa 54
100 5 4.6 MPa 46
100 8 7.1 MPa 71
200 5 2.3 MPa 23
200 8 3.7 MPa 37

How to read this table. These are pressures at which the inner-wall stress would reach the design stress at room temperature. They are not allowable working pressures. A real design stays well below them to leave margin for flaws, sustained load, cycling, temperature and the stresses at the ends. Notice that a 200 mm ID tube with a 5 mm wall reaches the limit at about half the pressure of a 100 mm ID tube with the same wall: diameter hurts.

Worked example. A 100 mm ID tube with a 3 mm wall (ri = 50 mm, ro = 53 mm) runs at 0.3 MPa (3 bar) gauge. The Lamé factor is (532 + 502) / (532 − 502) = 17.2, so the inner-wall stress is about 0.3 × 17.2 = 5.2 MPa. That is roughly one tenth of the 48 MPa design stress. This is comfortable for the wall itself, and the weak points then become the flanges, ports and seals.

Vacuum and external pressure: buckling, not crushing

Under external pressure the wall is in compression, and fused silica is very strong in compression (1,100 MPa). So a vacuum tube does not fail by crushing. It fails by buckling, when the circular cross-section collapses inward. The classical elastic buckling pressure for a long, perfectly round tube is:

Pcr = 2E / (1 − ν2) × (t / D)3

where E is Young’s modulus, ν is Poisson’s ratio, t is wall thickness and D is mean diameter. The cube on t/D is the key point: thin walls on large diameters lose stiffness very quickly. One atmosphere of vacuum is 0.101 MPa.

OD (mm) Wall (mm) Ideal buckling pressure Compared with 1 atm
50 2 10.7 MPa about 106×
100 3 4.4 MPa about 43×
200 3 0.52 MPa about 5×
300 4 0.37 MPa about 3.6×
500 3 0.033 MPa about 0.3×
500 8 0.64 MPa about 6×
1000 8 0.078 MPa about 0.8×
1000 12 0.27 MPa about 2.6×

Two lessons come out of this table. First, ordinary small and medium tubes have a very large buckling margin under 1 atm of vacuum. Second, large-diameter thin-wall tubes do not. A 500 mm OD tube with a 3 mm wall, or a 1,000 mm OD tube with an 8 mm wall, is below the ideal buckling pressure at 1 atm of external load, before any real-world reduction.

The formula assumes a perfectly round, long, unsupported tube at room temperature. Real tubes are slightly oval, and ovality lowers the buckling pressure. Short tubes and tubes with end rings or supports are stiffer than the formula says. So use it to screen, apply a generous factor, and ask the manufacturer to confirm. If you work with large tubes, read our guide to large-diameter quartz tubes as well.

What temperature does to the numbers

Every calculation above is a room-temperature screening value. At furnace temperature three things change:

  • Creep. Fused silica is continuous to about 1,200 °C and softens near 1,680 °C. Close to the upper end of the service range a wall under load, especially under external pressure, can slowly deform. We ask customers to flag surfaces that run above about 1,150 °C so we can review the wall and support.
  • Thermal stress. Fused silica has a very low expansion coefficient, but gradients still make stress. As a rough estimate, a fully constrained surface layer sees about 0.048 MPa per kelvin of temperature difference (E × α / (1 − ν)), which is about 4.8 MPa for a 100 K gradient. That is small against 48 MPa, but it adds to pressure stress and is not negligible in thick walls or fast ramps.
  • Chemistry. Hot alkali vapors and some other contaminants attack the surface, create devitrified patches and open the flaws that set the strength. See our overview of high-temperature quartz applications.

A pressure or vacuum rating is therefore stated at a temperature, and you should state your temperature profile in the request, not only the peak.

The weak points are usually not the straight wall

In pressurized and vacuum systems the straight tube is often the strongest part. Failures start at:

  • Flanges, ports and branches. Openings concentrate stress. Fused and machined flanges are built differently; our article on flanged quartz tube joints explains the options.
  • Welds. A flame-welded joint is a local thermal history and must be annealed to remove residual stress. See flame-welded joints on fused silica.
  • Clamps and seals. Metal-to-glass point loads and over-tightened clamps put tension where the glass cannot take it. Use compliant gaskets and spread the load.
  • Surface damage. Edges and ends that are only cut are more vulnerable than fire-polished ones. Fire polishing is available on our tubes, and any pressure part should have its handling and cleaning defined.

Annealed and polished parts also have lower residual stress, which is why pressure and vacuum tubes are usually specified with finished ends. Our custom quartz glass page lists the flame forming, welding and finishing available.

What to send with your request

To get a wall thickness confirmed rather than guessed, include:

Item Why it matters
Maximum internal pressure, and whether it is gauge or absolute Sets hoop stress
Vacuum level and any external pressure Sets buckling margin
Steady or cycling, and cycles per day Sustained and cyclic loads need more margin
Temperature profile, including ramp rates Sets creep and thermal stress
Process gases or liquids Surface attack and devitrification risk
ID or OD, wall if you have a target, and length Geometry for both calculations
End and port design, flanges, seals Where stress concentrates
Support points, orientation and mounting Bending and point loads
Quantity and inspection or documentation needs Planning and verification

A drawing or sketch is enough to start; single prototypes are fine, and we confirm critical dimensions in design-for-manufacture review before cutting glass. You can send a drawing for a quote.

When quartz alone is the wrong answer

If your design needs high sustained pressure at very high temperature, or the failure of a glass tube would be dangerous, a common solution is a metal or ceramic pressure shell with a quartz liner or insert, so the quartz carries the chemistry and temperature and the shell carries the pressure. We would rather tell you that before you buy than after. Pressure equipment rules differ by country and by application, so check which rules apply to your whole assembly.

Frequently asked questions

How much pressure can a quartz tube withstand?

It depends on diameter, wall thickness, temperature, surface condition and load type. As a screening example, a 50 mm ID tube with a 3 mm wall reaches the 48 MPa design stress at about 5.4 MPa internal pressure at room temperature. A real working pressure is much lower and should be confirmed for the exact tube.

Can a quartz tube be used under vacuum?

Yes, and standard small and medium tubes have a large buckling margin at 1 atm. Large-diameter, thin-wall tubes can be limited by buckling, so check the wall thickness against the buckling formula and ask for confirmation.

Does a thicker wall always mean a higher pressure rating?

For pressure, yes, up to a point. But a thicker wall also carries a larger temperature gradient and thermal stress, so thickness is a balance, not a free upgrade.

Is the pressure rating the same at 1,000 °C as at room temperature?

No. Rating is specified at a temperature, and creep and thermal stress reduce the margin as temperature rises. State your temperature profile.

What tensile strength should I use for design?

A common design value for fused silica is about 48 MPa (7,000 psi). It is a design value, not a guaranteed failure limit, and a flawed or long-loaded surface can fail lower, so you still need a safety factor on top of it.

Does FGQuartz supply tubes for pressure or vacuum service?

Yes, we make tubes from 5 to 1,000 mm OD with walls from 0.5 to 20 mm and more, including heavy-wall options for vacuum, and we calculate the wall for each drawing. See the quartz glass tubes page, or the quartz inline heaters page for flow-through chambers.

Next step: send FGQuartz your pressure, vacuum and temperature conditions with a sketch, and we will review wall thickness, ends and support in design-for-manufacture before any glass is cut.