Fabrication guide
How fused quartz is machined and flame-formed, which route suits each feature, and the design rules that reduce breakage, cost and lead time for custom quartz parts.
Quick Answer: Fused quartz is machined with diamond tools, not cut like metal. Holes, slots, flats, pockets and outlines are made by diamond CNC machining, grinding and polishing, while bends, closed ends, side arms and joints are made by oxy-hydrogen flame forming and welding. The material is hard and brittle, so good quartz designs avoid sharp inside corners, unneeded tight tolerances, thin deep features and load-bearing threads.
- Cold processing (diamond CNC, grinding, lapping, polishing) makes precise features and surfaces.
- Thermal processing (flame forming, welding, fire polishing, annealing) makes shapes that cannot be machined and relieves stress.
- Design for the tool. Add radii, chamfers or bevels, and call out tolerances only where the function needs them.
- Send the drawing early. A design-for-manufacture review before cutting is the cheapest way to avoid a redesign.
Written by the FGQuartz Engineering Team · Updated November 2026
On this page: Why quartz is different · Cold or thermal · Cold processing · Thermal processing · Design rules · Cost and lead time · What to send · FAQ
Why fused quartz machines differently from metal
Fused quartz is a hard, brittle glass. Its Mohs hardness is about 5.5 to 6.5, and producers list a Knoop hardness of roughly 520 kg/mm² for fused silica. It does not yield plastically the way metal does. When a cutting tool overloads it, it chips or cracks instead of deforming.
That has practical consequences:
- Diamond tooling is required. Carbide and steel tools wear out or fail. Diamond saws, drills, end mills and grinding wheels cut it, with coolant to carry heat and debris away.
- No single-point turning. A lathe tool cannot be used as on metal. Round parts are ground, and long tubes and rods are made by drawing and then finished.
- Damage lies below the surface. Aggressive cutting leaves micro-cracks that can later grow under thermal cycling or load. Finishing steps are chosen to remove or seal them.
- Low expansion helps. Fused quartz expands very little when heated by cutting, which is one reason it holds shape well during fabrication.
For the material itself, see what is quartz glass and the technical specifications.
Cold or thermal: which route makes which feature
FGQuartz uses two routes that work together: cold processing, which removes material with diamond tools, and thermal processing, which forms and joins glass in a flame. The feature usually decides the route.
| Feature | Usual route | Notes |
|---|---|---|
| Through holes, slots, flats, pockets, steps | Cold: diamond CNC, core drilling, milling | Radii and edge treatment set by the tool |
| Plate outlines, windows, discs | Cold: cutting, grinding, polishing | Finish from ground to optically polished |
| Precise OD, tight straightness | Cold: centerless grinding | Used when drawn tolerance is not enough |
| Bends, closed or domed ends, tapers | Thermal: flame forming | Annealed after forming |
| Side arms, ports, tees, manifolds | Thermal: flame forming and welding | Annealed after welding |
| Joining parts into an assembly | Thermal: flame welding | See flame-welded joints on fused silica |
| Smoothing and sealing edges | Thermal: fire polishing | Seals micro-cracks, reduces particle shedding |
The two routes are often combined. A slotted boat, for example, is slotted by CNC, welded to end plates in a flame and fire-polished at the slot edges. Our custom quartz glass page lists the capability matrix, and the guide to flame-welded joints on fused silica covers joining.
Cold processing: cutting, drilling, grinding and polishing
Cold processing starts from tube, rod, plate or block and removes material with diamond tools.
- Cutting. Diamond saws and wires cut stock to length and outline. Feed and coolant control chipping at the exit edge.
- Drilling and milling. Core drills make holes, and diamond end mills cut slots, pockets and steps. The tool radius limits the smallest inside corner.
- Grinding. Wheels bring dimensions, flatness and parallelism to the drawing, including centerless grinding of outside diameters.
- Lapping and polishing. Fine abrasives and polishing slurries produce the surfaces that optical and sealing parts need.
The surface finish is a specification, not a default:
| Finish | How it is made | Typical use |
|---|---|---|
| As-cut | Diamond cutting only | Hidden surfaces, non-critical parts |
| Fine-ground | Grinding | Dimensional control, seats, mounting faces |
| Fire-polished | Flame finishing | Edges and ends, to seal micro-cracks |
| Polished | Lapping and polishing | Windows, optical and sealing surfaces |
Plate parts and windows follow the same rules, with details on the quartz glass plate page.
Thermal processing: forming, welding, fire polishing and annealing
Thermal processing uses an oxy-hydrogen flame to soften the glass so it can be shaped and joined.
- Flame forming. Bends, domed or closed ends, tapers, necks and side arms are formed from tube and rod.
- Welding. Parts are fused into one piece: tube to tube, tube to plate, plate to plate. A welded joint is part of the glass, not a gasket.
- Fire polishing. A brief flame pass smooths edges and ends and seals surface micro-cracks left by cutting.
- Annealing. After forming or welding, parts are annealed to relieve internal stress, because residual stress can crack a part later in service.
Flame-worked tubes are covered on our quartz glass tubes page, and flanged joints in the article on flanged quartz tube joints.
Design rules that make quartz parts cheaper and stronger
These rules come from the way brittle glass behaves. Confirm limits for your size and feature in a design-for-manufacture review.
| Topic | Rule | Why |
|---|---|---|
| Inside corners | Avoid sharp inside corners and add a fillet. A fillet radius of at least about 0.5 mm at the bottom of pockets is a commonly cited minimum for glass | Sharp corners concentrate stress and start cracks. The tool has a radius, so a true sharp corner cannot be cut |
| Outside edges | Chamfer or bevel edges. A maximum bevel call-out, such as 0.5 mm max, is cheaper than a tight bevel tolerance | Sharp edges chip in handling and mounting. Over-tight edge tolerances slow production |
| Corners of plates | Use a bevel instead of a radius unless the radius must match a seal or pocket | Radius corners need extra CNC setups and slow feeds |
| Holes | Keep holes away from edges and from each other, and give the drilling side and exit side | Thin bridges between features crack. Breakout chips form at the exit |
| Thin walls and deep slots | Avoid them unless the function needs them, and ask about the limit | They flex and chip under tool load, and they increase scrap |
| Threads | Use sparingly and do not rely on them to carry load | Glass threads are weak compared with metal threads |
| Tolerances | State tight tolerances only on the surfaces that mate or seal, and call out the rest as general | Tolerance drives time, inspection and cost |
| Surface finish | Specify polish only on the faces that need it | Polishing is a separate, slower operation |
The most valuable habit is to send the drawing before it is final. A short review often changes a corner or a tolerance and saves a redesign.
What drives cost and lead time
- Number and type of features. Every hole, slot and pocket is a tool setup.
- Tolerances and finish. Tight tolerances and polished surfaces add machine time and inspection.
- Size and wall. Large or thin parts need slower feeds and more care.
- Welded assemblies. More joints mean more flame work and annealing.
- Grade. Optical and low-impurity grades and opaque fused silica are specified when the application needs them.
- Quantity. A prototype and a production run are planned differently, and prototypes start from one piece.
Simpler custom parts typically ship in 7 to 14 days, and complex custom assemblies take about 3 to 6 weeks. The quote confirms the schedule for your drawing.
What to send for a custom quartz part
| Item | What to include |
|---|---|
| Drawing | DXF, STEP, IGES or PDF, or a dimensioned sketch, sample or written description of the function |
| Critical dimensions | The surfaces that mate, seal or fit, with tolerance |
| Material and grade | Clear or opaque, process grade or optical grade, any purity limits |
| Finish | As-cut, ground, fire-polished or polished, and on which faces |
| Operating conditions | Temperature, atmosphere, pressure or vacuum, thermal cycling |
| Quantity and schedule | Prototype or production, and any deadline |
Free engineering review and NDA protection are available, and there is no minimum order quantity.
Frequently asked questions about machining fused quartz
Short answers written to stand alone.
Can fused quartz be machined?
Yes. Fused quartz is machined with diamond tools by cutting, core drilling, CNC milling, grinding, lapping and polishing. It is hard and brittle, so it cannot be turned with a single-point tool like metal, and every operation has to avoid chipping and cracking.
What tools are used to machine fused quartz?
Diamond tooling with coolant. Diamond saws and wires cut it, core drills make holes, diamond end mills and grinding wheels shape it, and abrasive slurries lap and polish it. Metal-cutting carbide tools do not work.
Can fused quartz be CNC machined?
Yes. CNC diamond machining is a standard route for holes, slots, flats, pockets, steps and profiles, with the toolpath and feeds set to protect the edges. Features that need bending, closing or joining are made by flame working instead.
Can you thread quartz glass?
Threads can be made in fused silica, but they are weak compared with metal threads and are not suited to carrying load. Use quartz threads for light closures and alignment, and design the load path through other parts.
When is flame working used instead of machining?
Flame working, with an oxy-hydrogen torch, forms bends, closed or domed ends, side arms and tapers, and welds parts together. Machining is better for holes, slots, flats, pockets and precise outlines. Many parts use both, and flame-worked parts are annealed afterward.
Why are sharp inside corners a problem in quartz?
Sharp inside corners concentrate stress and are where cracks start, and the tool that cuts them has a radius, so a true sharp corner is not possible. Specify a corner or fillet radius that suits the tool and the load.
What tolerances can be held when machining fused quartz?
Tolerances are set from the drawing and confirmed in design-for-manufacture review, because they depend on size, shape, feature and surface finish. Tolerances that are not needed raise cost, so call them out only where the fit or function requires them.
What should I send for a custom quartz part?
A drawing in DXF, STEP, IGES or PDF, or a dimensioned sketch, sample or written functional description. Include the critical dimensions, material grade, finish, operating temperature and quantity. A single prototype is a normal request.
Send the drawing, and we will review the route
Send the drawing or sketch with the critical dimensions, grade, finish and operating conditions. The engineering team reviews which features are machined, which are flame-formed, and where a change would cut cost or risk before any glass is cut. Quotes are typically returned within 24 business hours, and prototypes start from a single piece.